论文部分内容阅读
利用Gleeble-3500热模拟试验机,测定了Φ406.4 mm×16.5 mm X70深海无缝管线钢管(/%:0.07C,0.70Si,0.80Mn,0.008P,0.002S,0.25Ni,0.25Cr,0.20Mo,0.10Cu,0.06V,0.03Nb,0.04Alt,0.0060N)的CCT曲线,并通过光学显微镜,扫描电子显微镜,HV硬度计分析了0.1~100℃/s的冷却速度下钢管的组织特征。结果表明,冷却速度为0.1~5℃/s时钢中组织主要为铁素体+珠光体,当冷却速度大于5℃/s时