试验用A36和含Ce的A36Ce船板钢(/%:0.12~0.13C,0.21Si,0.77~0.79Mn,0.013 ~ 0.015P,0.003~0.004S,0.32~0.33Cr,0.023~0.025Al,0 ~0.009Ce)由真空感应炉熔炼,铸成7 kg锭,锻成25 mm×25 mm方坯,并经865℃0.5h空冷的正火处理.通过对普通不含Ce的A36船板钢和含0.009% Ce的A36Ce船板钢在模拟海水(3.5% NaCl)环境中的全浸试验,用失重、电化学方法、扫描电镜和X-射线衍