论文部分内容阅读
摘要:对新疆某复合铁矿石进行了选矿工艺试验研究。结果表明:采用先磁选后浮选的原则工艺流程,即将矿石矿磨至65%-200 目,进行铁粗选,铁粗精矿再磨至98%-200 目,两次精选,产出铁精矿,所得中矿及磁选尾矿合并作为给矿,通过添加丁基黄药和2#油进行选钴硫浮选,产出钴硫精矿及尾矿的工艺流程。产出的铁精矿品位为65.4%,回收率为81.57%,含硫 0.20%。钴硫精矿钴品位为0.21%,回收率为69.13%;硫品位为41.24%,回收率为93.75%。
关键词:复合铁矿石;先磁后浮;工艺流程
Abstract: The mineral processing experimental research was carried out on a composite Iron Ore of Xinjiang. The results showed that using the technological flowsheet of magnetic separation-flotation processed the ores.That is the composite Iron Ore was roughed under grinding to the size of 65%-74μm, and through iron roughing concentrate regrinding to the size of 98%-74μm iron concentrate was obtained with twice cleaning.The mine as consolidated middling and magnetic separation tailings obtained Cobalt pyrite concentrate though cobalt sulfide flotation by adding butyl xanthate and 2# oil.TFe grade of iron concentrate is 65.4%, iron recovery was 81.57% , Sulfur content was 0.20%. Cobalt grade of Cobalt pyrite concentrate was 0.21%,Cobalt recovery was 69.13%.Sulfur grade was41.24%,Sulfur recovery was 93.75%.
Key words: composite Iron Ore;magnetic separation-flotation;technological flowsheet
新疆某复合铁矿区位于新疆尼勒克县养鹿场南侧。依据地质详查资料,本矿已是国内待开发的中型铁矿,已探明的地质储量4651.57万吨[1] , 矿石中主要矿物成份为Fe,以磁性铁mFe为主,矿石全铁品位22.23~52.16%。脉石矿物主要为碳酸盐和石英,碳酸盐呈团块状、细网脉状集合体分布于磁铁、黄铁矿之间。同时,矿石中所含的铜、钴、银等元素的含量均达不到伴生矿的品位要求,但S、SiO2的含量超标,对磁法选矿有较大影响[2]。为合理开发该类型矿产资源,最大限度地综合回收资源,作者对新疆某复合铁矿石开展了详细的矿石性质及可选性试验研究工作[3-7],希望能为该矿矿产资源的综合利用提供有效指导,也为矿石的选矿方法和选矿流程提供可靠依据。
4 选矿试验
4.1 试验内容及流程
通过对该矿石进行的工艺矿物学研究表明,该矿石中铁矿物以磁铁矿为主,磁铁矿与脉石矿物嵌布关系紧密,并与金属硫化矿如黄铁矿、黄铜矿的嵌布关系也较为紧密。试验确定该矿石采用先磁选后浮选的原则工艺流程,将原矿磨至65%-200 目,进行铁粗选,铁粗精矿再磨至98%—200目,两次精选,产出铁精矿,所得中矿及磁选尾矿合并作为给矿,通过添加丁基黄药和2#油进行钴硫浮选,产出钴硫精矿及尾矿的工艺流程。
5 试验结论
1)矿石中主要矿物是磁铁矿,其次是磁赤铁矿、赤铁矿、褐铁矿、黄铁矿、黄铜矿、铜兰等。脉石矿物主要是透闪石、阳起石、绿帘石、绿泥石、石榴石、石英、方解石等。
2)通过对该矿石进行的工艺矿物学研究表明,磁铁矿与脉石矿物嵌布关系紧密,并与金属硫化矿如黄铁矿、黄铜矿的嵌布关系也较为紧密。
3)该矿石采用先磁选后浮选的原则工艺流程。即将原矿磨至65%-200 目,进行铁粗选,铁粗精矿再磨至98%-200 目,两次精选,产出铁精矿,所得中矿及磁选尾矿合并作为给矿,通过添加丁基黄药和2#油进行选钴硫浮选,产出钴硫精矿及尾矿的工艺流程。该矿石采用先磁后浮的工艺方案获得了较好的试验指标,产出的铁精矿品位为65.4%,回收率为81.57%,含硫 0.20%;钴硫精矿钴品位为0.21%,回收率为69.13%;硫品位为41.24%,回收率为93.75%。
参考文献
[1] 新疆地质矿产勘查开发局第七地质大队.新疆尼勒克县松湖铁矿详查报告[R].新疆尼勒克县:新疆天华矿业有限责任公司,2008.
[2] 钟向东,周慧平.复杂难选铁矿石选矿工艺的研究与实践[J].矿业快报,2008(6):66—69.
[3] 《矿产资源综合利用手册》编辑委员会.矿产资源综合利用手册[M].北京:科学出版社,1999.
[4] 徐国风.矿相学教程[M].武汉:武汉地质学院出版社,1986.
[5] 邱廷省,罗仙平,方夕辉.黄铁矿氧化抑制行为及机理研究[J].矿产综合利用,2001,10(5):17—19.
[6] 毛国胜,贾增良.低硫磁铁矿石综合利用研究[J].有色金属(选矿部分),2004(6)25—26.
[7] 孙传尧.复杂难处理矿石选矿技术[C]//全国选矿学术会议论文集.北京:冶金工业出版社,2009: 170-173.
关键词:复合铁矿石;先磁后浮;工艺流程
Abstract: The mineral processing experimental research was carried out on a composite Iron Ore of Xinjiang. The results showed that using the technological flowsheet of magnetic separation-flotation processed the ores.That is the composite Iron Ore was roughed under grinding to the size of 65%-74μm, and through iron roughing concentrate regrinding to the size of 98%-74μm iron concentrate was obtained with twice cleaning.The mine as consolidated middling and magnetic separation tailings obtained Cobalt pyrite concentrate though cobalt sulfide flotation by adding butyl xanthate and 2# oil.TFe grade of iron concentrate is 65.4%, iron recovery was 81.57% , Sulfur content was 0.20%. Cobalt grade of Cobalt pyrite concentrate was 0.21%,Cobalt recovery was 69.13%.Sulfur grade was41.24%,Sulfur recovery was 93.75%.
Key words: composite Iron Ore;magnetic separation-flotation;technological flowsheet
新疆某复合铁矿区位于新疆尼勒克县养鹿场南侧。依据地质详查资料,本矿已是国内待开发的中型铁矿,已探明的地质储量4651.57万吨[1] , 矿石中主要矿物成份为Fe,以磁性铁mFe为主,矿石全铁品位22.23~52.16%。脉石矿物主要为碳酸盐和石英,碳酸盐呈团块状、细网脉状集合体分布于磁铁、黄铁矿之间。同时,矿石中所含的铜、钴、银等元素的含量均达不到伴生矿的品位要求,但S、SiO2的含量超标,对磁法选矿有较大影响[2]。为合理开发该类型矿产资源,最大限度地综合回收资源,作者对新疆某复合铁矿石开展了详细的矿石性质及可选性试验研究工作[3-7],希望能为该矿矿产资源的综合利用提供有效指导,也为矿石的选矿方法和选矿流程提供可靠依据。
4 选矿试验
4.1 试验内容及流程
通过对该矿石进行的工艺矿物学研究表明,该矿石中铁矿物以磁铁矿为主,磁铁矿与脉石矿物嵌布关系紧密,并与金属硫化矿如黄铁矿、黄铜矿的嵌布关系也较为紧密。试验确定该矿石采用先磁选后浮选的原则工艺流程,将原矿磨至65%-200 目,进行铁粗选,铁粗精矿再磨至98%—200目,两次精选,产出铁精矿,所得中矿及磁选尾矿合并作为给矿,通过添加丁基黄药和2#油进行钴硫浮选,产出钴硫精矿及尾矿的工艺流程。
5 试验结论
1)矿石中主要矿物是磁铁矿,其次是磁赤铁矿、赤铁矿、褐铁矿、黄铁矿、黄铜矿、铜兰等。脉石矿物主要是透闪石、阳起石、绿帘石、绿泥石、石榴石、石英、方解石等。
2)通过对该矿石进行的工艺矿物学研究表明,磁铁矿与脉石矿物嵌布关系紧密,并与金属硫化矿如黄铁矿、黄铜矿的嵌布关系也较为紧密。
3)该矿石采用先磁选后浮选的原则工艺流程。即将原矿磨至65%-200 目,进行铁粗选,铁粗精矿再磨至98%-200 目,两次精选,产出铁精矿,所得中矿及磁选尾矿合并作为给矿,通过添加丁基黄药和2#油进行选钴硫浮选,产出钴硫精矿及尾矿的工艺流程。该矿石采用先磁后浮的工艺方案获得了较好的试验指标,产出的铁精矿品位为65.4%,回收率为81.57%,含硫 0.20%;钴硫精矿钴品位为0.21%,回收率为69.13%;硫品位为41.24%,回收率为93.75%。
参考文献
[1] 新疆地质矿产勘查开发局第七地质大队.新疆尼勒克县松湖铁矿详查报告[R].新疆尼勒克县:新疆天华矿业有限责任公司,2008.
[2] 钟向东,周慧平.复杂难选铁矿石选矿工艺的研究与实践[J].矿业快报,2008(6):66—69.
[3] 《矿产资源综合利用手册》编辑委员会.矿产资源综合利用手册[M].北京:科学出版社,1999.
[4] 徐国风.矿相学教程[M].武汉:武汉地质学院出版社,1986.
[5] 邱廷省,罗仙平,方夕辉.黄铁矿氧化抑制行为及机理研究[J].矿产综合利用,2001,10(5):17—19.
[6] 毛国胜,贾增良.低硫磁铁矿石综合利用研究[J].有色金属(选矿部分),2004(6)25—26.
[7] 孙传尧.复杂难处理矿石选矿技术[C]//全国选矿学术会议论文集.北京:冶金工业出版社,2009: 170-173.