论文部分内容阅读
为探究皂化棉籽油脚与改性膨润土复合的最佳工艺,通过单因素试验和正交试验研究分析了膨润土添加量、皂化棉籽油脚添加量、棉籽油添加量、搅拌时间和搅拌温度对复合工艺的影响。结果表明,最佳工艺参数为膨润土添加量1.0 g、皂化棉籽油脚添加量1.5 g、棉籽油添加量3 mL、搅拌温度80℃、搅拌时间1.0h,产品满足相关技术要求。
In order to explore the best technology of compounding saponified cottonseed oil with modified bentonite, the effects of adding amount of bentonite, adding amount of saponified cottonseed oil, adding amount of cottonseed oil, mixing time and stirring temperature to the composite were studied by single factor test and orthogonal experiment. The impact of technology. The results showed that the optimum technological parameters were 1.0 g bentonite, 1.5 g saponified cottonseed oil, 3 mL cottonseed oil, 80 ℃ stirring time and 1.0h stirring time. The products meet the relevant technical requirements.