论文部分内容阅读
【摘 要】外墙饰面砖粘结强度的质量现状,粘结强度偏低质量问题的危害性,造成外墙饰面砖粘结强度质量问题的原因分析,保证外墙饰面砖粘结强度质量的措施和建议。
【关键词】外墙饰面砖;粘结强度;质量问题;危害性;原因分析;保证措施
Strength quality control measures for outside wall decoration surface brick glues
Zhang Hong-guan
(Fushun zhongyu Construction(group) limited liability company Fushun Liaoning 113000)
【Abstract】Outside wall decoration the surface brick glue to knot the quality present condition of strength and glue the bane of knot strength low quality problem and result in outside wall decoration the surface brick glue to knot reason of the problem of strength quality analysis and promise an outside wall decorate the surface brick glue to knot the measure and suggestion of strength quality.
【Key words】Outside wall decorate surface brick; Glue knot strength; Quality problem; Endanger ; Reason analysis; Control measures
1. 外墙饰面砖粘贴强度不合格质量问题的危害性
外墙饰面砖由于具有装饰效果美观大方、颜色耐久性好、规格型号多种多样、价格区间大及施工方便等优点,因此,从80年代后期开始,外墙装饰采用饰面砖的工程迅速增多。与此同时,因外墙饰面砖粘贴强度不合格质量问题引起的饰面砖空鼓、饰面砖脱落伤人及物等质量安全事故也时有发生,许多很美观大方的建筑物因饰面砖的脱落而变得面目全非。因此,外墙饰面砖粘贴强度不合格质量问题属于严重的质量安全隐患,不仅影响到建筑物及环境的美观,而且关系到人民生命财产的安全。
《建筑装饰装修工程质量验收规范》(GB50210—2001)第8.3.4条规定:“饰面砖粘贴必须牢固”,这是一条强制性条文,必须严格执行。因此,外墙饰面砖粘结强度不合格的工程不得通过验收,否则属于违背国家建设工程强制性标准的行为,应进行维修和返工处理。然而饰面砖的维修和返工非常困难,属于高空作业,安全费用及维修费用较高。由此可见,外墙饰面砖粘贴强度不合格质量问题具有较大的危害性,应引起有关责任主体单位特别是施工单位的高度重视。
2. 外墙饰面砖质量现状
目前,检测外墙饰面砖粘贴强度所采用的标准是行业标准《建筑工程饰面砖粘结强度检验标准》(JGJ110—97)。按照该标准第6.0.1、6.0.3条规定:在建筑物外墙上镶贴的同类饰面砖,其粘结强度同时符合以下两项指标时可定为合格:
(1)每组试样平均粘结强度不应小于0.4MPa;
(2)每组可以有一个试样的粘结强度小于0.4MPa,但不应小于0.3MPa。
当两项指标均不符合要求时,其粘结强度应定为不合格。
当只有其中一项指标不符合要求时,应在该组试样原取样区域内重新抽取双倍试样检验。若检验结果仍有一项指标达不到规定数值,则该批饰面砖粘结强度可定为不合格。按照该标准附录B的规定,饰面砖试件破坏状态共分八种,分别是:(1)粘结剂与饰面砖界面破坏;(2)饰面砖破坏;(3)饰面砖与粘结层界面破坏;(4)粘结层破坏;(5)粘结层与找平层界面破坏;(6)找平层破坏;(7)找平层与基体界面破坏;(8)基体破坏。当测试结果为第(1)、(2)、(8)种破坏状态时,应重新选点测试,至出现第(3)种至第(7)种破坏状态之一时为止。
根据某检测机构对所在区域建筑工程外墙饰面砖粘结强度不合格率的统计资料显示,第(3)种至第(7)种破坏状态各自所占的比例如下:
a、第三种破坏状态,即饰面砖与粘结层界面破坏,在所有不合格的试件中所占比例达到28%;
b、第四种破坏状态,即粘结层破坏,在所有不合格的试件中所占比例达到40%;
c、第五种破坏状态,即粘结层与找平层界面破坏,在所有不合格的试件中所占比例达到10%;
d、第六种破坏状态,即找平层破坏,在所有不合格的试件中所占比例达到12%;
e、第七种破坏状态,即找平层与基体界面破坏,在所有不合格的试件中所占比例达到10%。
上述统计资料表明:外墙饰面砖粘贴强度破坏状态主要是第(3)种和第(4)种,两种情况合计不合格率近70%;第(5)、(6)、(7)三种破坏状态不合格率约30%。笔者对饰面砖脱落的建筑物进行观察发现:大部分饰面砖脱落的建筑物,基本上是饰面砖脱落;也有少部分是连找平层一起脱落的情况,与上述统计分析基本一致。因此,要提高外墙饰面砖粘贴强度的质量有两个环节,首先应该保证找平层的施工质量,防止第(6)、(7)种破坏状态发生;其次保证粘结层的施工质量,防止第(3)、(4)、(5)种破坏状态的发生。
3. 外墙饰面砖粘贴强度不合格质量问题原因分析
在工程建设中,影响工程产品质量的因素主要有“人、材料、机械、方法和环境”等五大方面,同样,影响外墙饰面砖粘贴强度质量也是这五大因素:
3.1 人的因素主要表现在施工及监理单位相关人员管理不到位、责任心不强、对此质量问题未引起足够重视以及操作工人的工艺水平较低、工艺不够熟练、施工经验欠缺等情况。按照《外墙饰面砖工程施工及验收规程》(JGJ126—2000、J23—2000)第5.1.3条的要求:外墙饰面砖工程施工前应做出样板,经建设、设计和监理等单位根据有关标准确认后方可施工。施工前,施工单位质量、技术负责人对操作班组长在施工工艺、施工技术和施工质量检测标准等方面进行交底。但很少有工地进行这些工作。
3.2 机械因素:外墙饰面砖粘贴主要靠手工操作,机械因素对于外墙饰面砖粘贴强度质量的影响相对较小,主要是找平层的砂浆配合比要准确、搅拌要均匀。
3.3 施工工艺和施工方法的影响主要表现在操作工人的施工工艺控制不好,造成水泥浆粘结层强度偏低以及水泥浆粘结层不饱满。按照《外墙饰面砖工程施工及验收规程》(JGJ126—2000、J23—2000)第5.2.5条的要求:在粘贴面砖前应对面砖进行挑选,浸水2小时以上并清洗干净,待表面晾干后方可粘贴;粘贴面砖时基层的含水率宜为15%~25%;当气温高于35°C时,应有遮阳设施;这些要求均是保证水泥浆粘结层强度的有效措施。同时,对基层的处理和找平层的施工工艺也存在缺陷,外墙饰面砖粘贴完毕后,12小时内没有进行养护。
3.4 原材料的影响主要表现在对进场各种原材料进行复验把关不严。按照《外墙饰面砖工程施工及验收规程》(JGJ126—2000、J23—2000)第5.1.1、5.1.2条的要求:(1)在外墙饰面砖工程施工前,应对各种原材料进行复验,外墙饰面砖应具有生产厂家的出厂检验报告及产品合格证。进场后应进行尺寸、表面质量、吸水率等项目的复检;(2)粘贴外墙饰面砖所用的水泥、砂、胶粘剂等材料均应进行复检,合格后方可使用;(3)在外墙饰面砖工程施工前,应队找平层、结合层、粘结层及勾缝、嵌缝所用的材料进行试配,经检验合格后方可使用。
3.5 环境影响。施工时的环境温度、湿度、日晒、雨淋等因素对外墙饰面砖粘贴强度质量的影响很大,因此,应避免在暴雨、暴晒的情况下进行粘贴施工。
4. 保证外墙饰面砖粘贴强度质量的措施
“外墙饰面砖粘贴必须牢固”属于强制性条文,必须严格执行。 特别是现在土地资源紧缺、建筑物高度将不断增高,外墙饰面砖粘结强度偏低质量安全隐患的严重性、危害性愈来愈大。针对上述外墙饰面砖粘贴强度偏低产生的原因,为保证外墙饰面砖粘贴强度质量,应采取以下措施:
4.1 强化施工质量管理 ,严格按照《外墙饰面砖工程施工及验收规程》(JGJ126-2000、J23-2000)和其它相关规范组织施工。外墙饰面砖在施工前应先做样板件,通过有关单位对样板件进行检测、验收合格后才大面积铺开粘贴。通过样板件的施工可以找出适合于不同墙体的施工工艺和施工方法;可以找出适合于不同墙体的找平层、粘结层材料品种;可以避免返工浪费的情况发生。特别是现在国家推行墙体改革和建筑节能政策,禁止使用粘土砖以后,各种新型墙体材料的品种层出不穷,同时为满足节能要求,墙体上需设置保温、隔热和防水层,使外墙的构造变得越来越复杂,通过样板件可以找出墙体各构造层之间的协调和匹配施工方法。同时,各相关规范对样板件都有明确规定,国家标准《建筑装饰装修工程质量验收规范》(GB50210-2001)第8.1.7条规定:外墙饰面砖粘贴前和施工过程中,均应在相同基层上做样板件,并对样板件的饰面砖粘贴强度进行检验,其检验方法和结果判定应符合《建筑工程饰面砖粘结强度检验标准》(JGJ110)的规定;行业标准《外墙饰面砖工程施工及验收规程》(JGJ126-2000、J23-2000)第5.1.3条的规定:外墙饰面砖工程施工前应做出样板,经建设、设计、和监理等单位根据有关标准确认后方可施工。
4.2 强化检测工作,外墙饰面砖粘结强度的检测点应选择在有代表性的部位进行。重要墙面没有检测、验收合格之前,不得拆除外脚手架。
按照《建筑工程饰面砖粘结强度检验标准》(JGJ110—97)第3.0.5条规定:采用水泥砂浆或水泥浆粘结时,应在水泥砂浆或水泥浆龄期达到28d时进行检验。当在7d或14d进行检验时,应通过对比试验确定其粘结强度的修正系数。因此,按照此要求,一般的外墙饰面砖粘结强度检测报告是以水泥砂浆或水泥浆龄期达到28d时的强度为标准。有很多工程为了赶工期,当水泥砂浆或水泥浆龄期未达到28d时就拆除了外脚手架。这样一来,外墙饰面砖粘结强度检测只能在检测人员方便、安全到达的外阳台内墙面、屋面楼梯间墙面、底层外墙面等部位进行,这些部位的墙面为一般墙面。这些部位的施工环境好、容易保证质量,因此其检测结果不具有代表性。即使这些部位检测结果不合格,其危害性较小、返工维修比较简单。因此,外墙饰面砖粘结强度的检测点应选择在有代表性的部位进行。重要墙面才是具有代表性的部位,所谓重要墙面就是只有通过外脚手架才能到达的墙面,直接面临繁华街道的墙面,受日照、温差、雨雪、冰冻、台风直接影响的墙面。百年大计、质量第一,按照《建筑装饰装修工程质量验收规范》(GB50210—2001)第8.3.4条强制性条文规定:“外墙饰面砖粘贴必须牢固”,外墙饰面砖粘结强度检测属于对建筑物进行使用安全的检测内容。因此,外墙饰面砖粘结强度的检测点应在规范划分的检验批范围内进行;在外脚手架未拆除之前进行;重要墙面没有检测、验收合格之前,不得拆除外脚手架。
4.3 强化检验批的验收,严格执行《建筑装饰装修工程质量验收规范》(GB50210-2001)和其它相关规范的规定,不打折扣。 “外墙饰面砖粘贴必须牢固”属于强制性条文,必须严格执行。因此,对外墙饰面砖检验批的验收应严格标准,不能流于形式、走一走过场。《建筑装饰装修工程质量验收规范》(GB50210-2001)第8.1.5条规定:各分项工程的检验批应按下列规定划分:相同材料、工艺和施工条件的室外饰面砖工程每500m2至1000m2应划分为一个检验批,不足500m2也应划分为一个检验批。按照《建筑工程饰面砖粘结强度检验标准》(JGJ110-97)第3.0.3条规定:现场镶贴的外墙饰面砖工程:每300m2同类墙体取1组试样,每组三个,每一楼层不得少于一组;不足300m2同类墙体,每两楼层取一组试样,每组三个。在实际操作时,对于重要墙面可按每300m2作为一个检验批;对于一般墙面可按每500m2至1000m2作为一个检验批。每一个检验批均进行一组拉拔试验,检测粘贴是否牢固,满粘法施工的饰面砖应检查有无空鼓、裂缝等主控项目,其它一般项目的检查也应按规范严格执行。对于饰面砖粘贴强度不合格、存在空鼓、裂缝等情况的检验批,坚决不予通过验收,返工重做直到符合要求为止。
[文章编号]1006-7619(2010)06-04-506
【关键词】外墙饰面砖;粘结强度;质量问题;危害性;原因分析;保证措施
Strength quality control measures for outside wall decoration surface brick glues
Zhang Hong-guan
(Fushun zhongyu Construction(group) limited liability company Fushun Liaoning 113000)
【Abstract】Outside wall decoration the surface brick glue to knot the quality present condition of strength and glue the bane of knot strength low quality problem and result in outside wall decoration the surface brick glue to knot reason of the problem of strength quality analysis and promise an outside wall decorate the surface brick glue to knot the measure and suggestion of strength quality.
【Key words】Outside wall decorate surface brick; Glue knot strength; Quality problem; Endanger ; Reason analysis; Control measures
1. 外墙饰面砖粘贴强度不合格质量问题的危害性
外墙饰面砖由于具有装饰效果美观大方、颜色耐久性好、规格型号多种多样、价格区间大及施工方便等优点,因此,从80年代后期开始,外墙装饰采用饰面砖的工程迅速增多。与此同时,因外墙饰面砖粘贴强度不合格质量问题引起的饰面砖空鼓、饰面砖脱落伤人及物等质量安全事故也时有发生,许多很美观大方的建筑物因饰面砖的脱落而变得面目全非。因此,外墙饰面砖粘贴强度不合格质量问题属于严重的质量安全隐患,不仅影响到建筑物及环境的美观,而且关系到人民生命财产的安全。
《建筑装饰装修工程质量验收规范》(GB50210—2001)第8.3.4条规定:“饰面砖粘贴必须牢固”,这是一条强制性条文,必须严格执行。因此,外墙饰面砖粘结强度不合格的工程不得通过验收,否则属于违背国家建设工程强制性标准的行为,应进行维修和返工处理。然而饰面砖的维修和返工非常困难,属于高空作业,安全费用及维修费用较高。由此可见,外墙饰面砖粘贴强度不合格质量问题具有较大的危害性,应引起有关责任主体单位特别是施工单位的高度重视。
2. 外墙饰面砖质量现状
目前,检测外墙饰面砖粘贴强度所采用的标准是行业标准《建筑工程饰面砖粘结强度检验标准》(JGJ110—97)。按照该标准第6.0.1、6.0.3条规定:在建筑物外墙上镶贴的同类饰面砖,其粘结强度同时符合以下两项指标时可定为合格:
(1)每组试样平均粘结强度不应小于0.4MPa;
(2)每组可以有一个试样的粘结强度小于0.4MPa,但不应小于0.3MPa。
当两项指标均不符合要求时,其粘结强度应定为不合格。
当只有其中一项指标不符合要求时,应在该组试样原取样区域内重新抽取双倍试样检验。若检验结果仍有一项指标达不到规定数值,则该批饰面砖粘结强度可定为不合格。按照该标准附录B的规定,饰面砖试件破坏状态共分八种,分别是:(1)粘结剂与饰面砖界面破坏;(2)饰面砖破坏;(3)饰面砖与粘结层界面破坏;(4)粘结层破坏;(5)粘结层与找平层界面破坏;(6)找平层破坏;(7)找平层与基体界面破坏;(8)基体破坏。当测试结果为第(1)、(2)、(8)种破坏状态时,应重新选点测试,至出现第(3)种至第(7)种破坏状态之一时为止。
根据某检测机构对所在区域建筑工程外墙饰面砖粘结强度不合格率的统计资料显示,第(3)种至第(7)种破坏状态各自所占的比例如下:
a、第三种破坏状态,即饰面砖与粘结层界面破坏,在所有不合格的试件中所占比例达到28%;
b、第四种破坏状态,即粘结层破坏,在所有不合格的试件中所占比例达到40%;
c、第五种破坏状态,即粘结层与找平层界面破坏,在所有不合格的试件中所占比例达到10%;
d、第六种破坏状态,即找平层破坏,在所有不合格的试件中所占比例达到12%;
e、第七种破坏状态,即找平层与基体界面破坏,在所有不合格的试件中所占比例达到10%。
上述统计资料表明:外墙饰面砖粘贴强度破坏状态主要是第(3)种和第(4)种,两种情况合计不合格率近70%;第(5)、(6)、(7)三种破坏状态不合格率约30%。笔者对饰面砖脱落的建筑物进行观察发现:大部分饰面砖脱落的建筑物,基本上是饰面砖脱落;也有少部分是连找平层一起脱落的情况,与上述统计分析基本一致。因此,要提高外墙饰面砖粘贴强度的质量有两个环节,首先应该保证找平层的施工质量,防止第(6)、(7)种破坏状态发生;其次保证粘结层的施工质量,防止第(3)、(4)、(5)种破坏状态的发生。
3. 外墙饰面砖粘贴强度不合格质量问题原因分析
在工程建设中,影响工程产品质量的因素主要有“人、材料、机械、方法和环境”等五大方面,同样,影响外墙饰面砖粘贴强度质量也是这五大因素:
3.1 人的因素主要表现在施工及监理单位相关人员管理不到位、责任心不强、对此质量问题未引起足够重视以及操作工人的工艺水平较低、工艺不够熟练、施工经验欠缺等情况。按照《外墙饰面砖工程施工及验收规程》(JGJ126—2000、J23—2000)第5.1.3条的要求:外墙饰面砖工程施工前应做出样板,经建设、设计和监理等单位根据有关标准确认后方可施工。施工前,施工单位质量、技术负责人对操作班组长在施工工艺、施工技术和施工质量检测标准等方面进行交底。但很少有工地进行这些工作。
3.2 机械因素:外墙饰面砖粘贴主要靠手工操作,机械因素对于外墙饰面砖粘贴强度质量的影响相对较小,主要是找平层的砂浆配合比要准确、搅拌要均匀。
3.3 施工工艺和施工方法的影响主要表现在操作工人的施工工艺控制不好,造成水泥浆粘结层强度偏低以及水泥浆粘结层不饱满。按照《外墙饰面砖工程施工及验收规程》(JGJ126—2000、J23—2000)第5.2.5条的要求:在粘贴面砖前应对面砖进行挑选,浸水2小时以上并清洗干净,待表面晾干后方可粘贴;粘贴面砖时基层的含水率宜为15%~25%;当气温高于35°C时,应有遮阳设施;这些要求均是保证水泥浆粘结层强度的有效措施。同时,对基层的处理和找平层的施工工艺也存在缺陷,外墙饰面砖粘贴完毕后,12小时内没有进行养护。
3.4 原材料的影响主要表现在对进场各种原材料进行复验把关不严。按照《外墙饰面砖工程施工及验收规程》(JGJ126—2000、J23—2000)第5.1.1、5.1.2条的要求:(1)在外墙饰面砖工程施工前,应对各种原材料进行复验,外墙饰面砖应具有生产厂家的出厂检验报告及产品合格证。进场后应进行尺寸、表面质量、吸水率等项目的复检;(2)粘贴外墙饰面砖所用的水泥、砂、胶粘剂等材料均应进行复检,合格后方可使用;(3)在外墙饰面砖工程施工前,应队找平层、结合层、粘结层及勾缝、嵌缝所用的材料进行试配,经检验合格后方可使用。
3.5 环境影响。施工时的环境温度、湿度、日晒、雨淋等因素对外墙饰面砖粘贴强度质量的影响很大,因此,应避免在暴雨、暴晒的情况下进行粘贴施工。
4. 保证外墙饰面砖粘贴强度质量的措施
“外墙饰面砖粘贴必须牢固”属于强制性条文,必须严格执行。 特别是现在土地资源紧缺、建筑物高度将不断增高,外墙饰面砖粘结强度偏低质量安全隐患的严重性、危害性愈来愈大。针对上述外墙饰面砖粘贴强度偏低产生的原因,为保证外墙饰面砖粘贴强度质量,应采取以下措施:
4.1 强化施工质量管理 ,严格按照《外墙饰面砖工程施工及验收规程》(JGJ126-2000、J23-2000)和其它相关规范组织施工。外墙饰面砖在施工前应先做样板件,通过有关单位对样板件进行检测、验收合格后才大面积铺开粘贴。通过样板件的施工可以找出适合于不同墙体的施工工艺和施工方法;可以找出适合于不同墙体的找平层、粘结层材料品种;可以避免返工浪费的情况发生。特别是现在国家推行墙体改革和建筑节能政策,禁止使用粘土砖以后,各种新型墙体材料的品种层出不穷,同时为满足节能要求,墙体上需设置保温、隔热和防水层,使外墙的构造变得越来越复杂,通过样板件可以找出墙体各构造层之间的协调和匹配施工方法。同时,各相关规范对样板件都有明确规定,国家标准《建筑装饰装修工程质量验收规范》(GB50210-2001)第8.1.7条规定:外墙饰面砖粘贴前和施工过程中,均应在相同基层上做样板件,并对样板件的饰面砖粘贴强度进行检验,其检验方法和结果判定应符合《建筑工程饰面砖粘结强度检验标准》(JGJ110)的规定;行业标准《外墙饰面砖工程施工及验收规程》(JGJ126-2000、J23-2000)第5.1.3条的规定:外墙饰面砖工程施工前应做出样板,经建设、设计、和监理等单位根据有关标准确认后方可施工。
4.2 强化检测工作,外墙饰面砖粘结强度的检测点应选择在有代表性的部位进行。重要墙面没有检测、验收合格之前,不得拆除外脚手架。
按照《建筑工程饰面砖粘结强度检验标准》(JGJ110—97)第3.0.5条规定:采用水泥砂浆或水泥浆粘结时,应在水泥砂浆或水泥浆龄期达到28d时进行检验。当在7d或14d进行检验时,应通过对比试验确定其粘结强度的修正系数。因此,按照此要求,一般的外墙饰面砖粘结强度检测报告是以水泥砂浆或水泥浆龄期达到28d时的强度为标准。有很多工程为了赶工期,当水泥砂浆或水泥浆龄期未达到28d时就拆除了外脚手架。这样一来,外墙饰面砖粘结强度检测只能在检测人员方便、安全到达的外阳台内墙面、屋面楼梯间墙面、底层外墙面等部位进行,这些部位的墙面为一般墙面。这些部位的施工环境好、容易保证质量,因此其检测结果不具有代表性。即使这些部位检测结果不合格,其危害性较小、返工维修比较简单。因此,外墙饰面砖粘结强度的检测点应选择在有代表性的部位进行。重要墙面才是具有代表性的部位,所谓重要墙面就是只有通过外脚手架才能到达的墙面,直接面临繁华街道的墙面,受日照、温差、雨雪、冰冻、台风直接影响的墙面。百年大计、质量第一,按照《建筑装饰装修工程质量验收规范》(GB50210—2001)第8.3.4条强制性条文规定:“外墙饰面砖粘贴必须牢固”,外墙饰面砖粘结强度检测属于对建筑物进行使用安全的检测内容。因此,外墙饰面砖粘结强度的检测点应在规范划分的检验批范围内进行;在外脚手架未拆除之前进行;重要墙面没有检测、验收合格之前,不得拆除外脚手架。
4.3 强化检验批的验收,严格执行《建筑装饰装修工程质量验收规范》(GB50210-2001)和其它相关规范的规定,不打折扣。 “外墙饰面砖粘贴必须牢固”属于强制性条文,必须严格执行。因此,对外墙饰面砖检验批的验收应严格标准,不能流于形式、走一走过场。《建筑装饰装修工程质量验收规范》(GB50210-2001)第8.1.5条规定:各分项工程的检验批应按下列规定划分:相同材料、工艺和施工条件的室外饰面砖工程每500m2至1000m2应划分为一个检验批,不足500m2也应划分为一个检验批。按照《建筑工程饰面砖粘结强度检验标准》(JGJ110-97)第3.0.3条规定:现场镶贴的外墙饰面砖工程:每300m2同类墙体取1组试样,每组三个,每一楼层不得少于一组;不足300m2同类墙体,每两楼层取一组试样,每组三个。在实际操作时,对于重要墙面可按每300m2作为一个检验批;对于一般墙面可按每500m2至1000m2作为一个检验批。每一个检验批均进行一组拉拔试验,检测粘贴是否牢固,满粘法施工的饰面砖应检查有无空鼓、裂缝等主控项目,其它一般项目的检查也应按规范严格执行。对于饰面砖粘贴强度不合格、存在空鼓、裂缝等情况的检验批,坚决不予通过验收,返工重做直到符合要求为止。
[文章编号]1006-7619(2010)06-04-506